Aluminum and Truck Wheel Polishing: Roundness, Fixturing, and Safety Compliance September 05 , 2026
Die-cast aluminium parts of the kind a wheel programme also runs — the thin-wall and ribbed sections are what make fixturing the hard part

Aluminum and Truck Wheel Polishing: Roundness, Fixturing, and Safety Compliance

Polishing Wheel Machine: Two Different Purchases

The phrase covers two machines that share a name and nothing else, and which one you want changes every answer on this page.

If you mean a bench or pedestal buffing machine

That is a single-spindle machine with a cloth wheel, used at a bench by an operator holding the part against the wheel. It is the right tool for one-off work, for restoring a finish by hand, and for parts too large or too few to justify a fixtured process. It is not what this page is about — and if that is your process, the compound question is the one that matters, not the machine.

If you mean a wheel (rim) polishing machine for automotive

That is the other purchase: a machine that finishes aluminium or alloy wheels in batch or on a fixture, where the constraints are roundness, run-out and how the wheel is held without distorting it. That is what this page covers — the two engineering constraints, the fixturing, the media progression and the takt-time question all belong to this second machine.

If you landed here looking for a bench buffer, the useful pages are the ones on [buffing compounds](/blog/buffing-compounds-for-metal-by-colour-and-by-metal/) and [polishing versus buffing as two operations](/blog/polishing-buffing-two-operations/). Everything below is about production wheel finishing, where the part is held and the process is measured.

Automotive cast aluminum wheels and heavy commercial forged truck wheels represent one of the most commercially valuable and technically unforgiving segments in industrial mass finishing. In procurement searches, terms like wheel polishing equipment, aluminum wheel polishing machine, and truck wheel polishing machine generate significant global inquiry. Yet manufacturing engineers, aftermarket refurbishers, and fleet maintenance directors routinely encounter superficial catalog literature. Most vendor websites treat wheel polishing as merely dropping a rim into an oversized vibratory tub or rotating it against an uncalibrated buffing spindle.

In high-volume manufacturing and precision wheel restoration, cosmetic shine is only the final verification step. Geometric roundness, critical datum preservation, and structural fatigue integrity are the prerequisites that govern whether a finished wheel is commercially acceptable or dangerously scrap.

A standard 19-inch cast passenger car wheel or a 22.5-inch forged truck wheel looks massive and rigid, but structurally it is a relatively thin-walled elastic shell. Clamping it incorrectly induces elastic deformation that results in out-of-round geometry upon release. Exposing mounting registers to abrasive slurry erodes precision center bores and lug nut tapers, compromising vehicle balance and fastener torque retention.

This comprehensive technical guide analyzes the structural constraints of wheel polishing equipment, details precision fixturing and datum masking, addresses the multi-stage media unloading challenge, resolves line takt-time bottlenecks, specifies environmental health and safety (EHS) aluminum sludge protocols, and establishes safety compliance standards for heavy commercial truck wheels under DOT and SAE J267 fatigue criteria.

Die-cast aluminium parts of the kind a wheel programme also runs — the thin-wall and ribbed sections are what make fixturing the hard part
Thin-walled aluminum castings and circular spoked structures. Notice the slender radial spoke ribs and precision bored center registers: aggressive, unmasked abrasive mass finishing will wash out critical bearing registers and erode spoke corner contours.

Two Engineering Constraints That Govern Wheel Polishing

Before specifying motor power, tub diameter, or abrasive pellets, production planners must recognize two physical realities that separate wheel polishing from general bracket or hardware finishing.

1. The Elastic Thin-Wall Phenomenon

An aluminum road wheel exhibits an outer diameter between 400 mm and 620 mm, while the rim barrel wall thickness frequently measures only 3.5 mm to 6.0 mm (varying by cast A356-T6 or forged 6061-T6 specification).

  • Clamping Distortion: If a heavy commercial truck wheel is clamped around its outer rim flange with rigid mechanical chuck jaws, the localized inward force deflects the hoop into an oval or tri-lobed shape during polishing. The abrasive cleans the high contact areas while missing the recessed valleys. When the clamping pressure is released post-process, the metal springs back elastically. The wheel emerges with measurable radial runout exceeding OEM limits (typically > 0.35 mm), causing permanent high-speed balance shudder on the vehicle.
  • Abrasive Pressure Gradients: In deep vibratory bowls, hydrostatic pressure from the fluidized media bed increases with depth. If the wheel orientation is static, the lower rim lip experiences significantly higher cutting aggression than the top face, resulting in asymmetric stock removal. Understanding how media circulation influences large circular envelopes is detailed in our guide to vibratory finishing machines and general deburring machine route selection.

2. Post-Process Geometric Measurement

Unlike decorative door handles or cookware where finishing quality is inspected purely with a 60° gloss meter, finished wheels must pass stringent dimensional and geometric inspection:

  1. Center Bore (CB) Runout and Tolerance: Typically specified as +0.05 / -0.00 mm. If abrasive slurry enters this register, the hub-centric fit is destroyed.
  2. Lug Nut Seat Geometry: 60° conical countersinks or spherical ball seats must maintain precise angularity to ensure proper wheel stud clamping preload without loosening under road vibration.
  3. Tire Bead Seat Profile: The bead seat profile must maintain strict radial circumference to ensure airtight tubeless tire bead seating without air seepage.

For an overview of how equipment forms dictate throughput across various spindle and station configurations, review wheel polishing equipment forms and line integration.

Precision Fixturing & Critical Surface Masking

The single greatest point of failure in automated aluminum wheel finishing is inadequate surface masking. If abrasive media is allowed to freely contact the rear mounting pad, bolt holes, or center bore, the wheel is ruined functionally regardless of how mirror-like the outer face appears.

```

Wheel Mounting Cross-Section & Masking Architecture:

[Front Rim Lip / Face / Spokes Exposed to Media Action] ──────────────────────────────────────────────────────────────── │ ▲ ▲ │ │ [Bolt Hole] [Bolt Hole] │ ▼ │ │ ▼ [Bead Seat Lip] ▼ ▼ [Bead Seat Lip] Masked on re-cut ┌───────────────┐ ┌───────────────┐ │ EPDM Plug │ │ EPDM Plug │ └───────────────┘ └───────────────┘ ▲ │ ┌─────────────────────────────────┐ │ Heavy-Duty Expanding Mandrel │ │ (Polyurethane Seal Block) │ │ Clamps securely inside CB │ └─────────────────────────────────┘ │ [Rear Mounting Pad: Hermetically Sealed via O-Ring Face Seal]

```

Center Bore and Hub Pad Protection

To isolate the center bore and rear mounting surface from abrasive wear:

  • Expanding Polyurethane Mandrels: The wheel is mounted via an internal expanding mandrel positioned within the central hub bore. The mandrel incorporates a heavy-duty Shore 90A polyurethane or vulcanized EPDM expanding sleeve. When actuated pneumatically or via a central drawbar, the sleeve expands radially against the rough cast interior of the hub recess, creating a hermetic seal against liquid compound and micro-fine abrasives.
  • Face O-Ring Seals: The rear mounting face is clamped firmly against a planar polyurethane backing plate equipped with dual concentric nitrile O-rings. This prevents chemical staining, micro-pitting, and abrasive erosion on the mating face that mounts flush against the vehicle brake rotor.

Lug Nut Countersink Masking

Lug nut holes (pitch circle diameter / PCD) must never be subjected to tumbling media:

  • Quick-Lock Masking Plugs: Custom injection-molded conical silicone or polyurethane plugs with internal through-bolts are fastened through each lug hole.
  • Taper Protection: The plugs seat tightly into the 60° conical bevel or spherical chamfer. This prevents abrasive rounding of the sharp edge transitions, guaranteeing that the wheel maintains proper torque retention when installed with pneumatic shop tools.

Valve Stem Hole Sealing

A standard valve stem aperture measures ⌀ 11.5 mm (or ⌀ 8.3 mm on specialized racing wheels). Media pellets matching this diameter will lodge tightly into the hole, causing rim damage during attempted punch-out. A dedicated expanding rubber core plug is locked into the valve aperture prior to charging the wheel into the finishing machine.

Three-Stage Media Progression and the Rapid Changeover Challenge

Achieving a high-luster commercial mirror finish on cast A356 or forged 6061-T6 aluminum requires a progressive three-stage mechanical finishing sequence.

Process Stage Primary Operational Objective Recommended Media Specification Process Liquid / Chemistry Typical Stage Duration Resulting Surface (Ra)
Stage 1: Primary Cut Level the CNC tool marks left by the previous turning pass, remove cast parting skin, radius the sharp spoke edges High-density polyester-bonded plastic cones or angle-cut triangles (120# – 180# grit) compound-LC10 (neutral surfactant/degreaser, 2% concentration) 90 to 150 minutes a uniform matte that reads even
Stage 2: Fine Smoothing Eradicate microscopic cutting scratches, prepare dense metallurgical skin for mirror burnishing Fine-mesh synthetic plastic media (320# – 600# grit) or fine porcelain cylinders compound-LC10 (continuous freshwater flush to clear swarf) 60 to 120 minutes a smooth surface with the cutting traces closed
Stage 3: Mirror Burnishing Cold-work micro-asperities via compressive micro-peening, achieve specular reflection High-density zirconia beads (⌀ 3 – 4 mm) or polished porcelain balls (⌀ 4 – 6 mm) compound-JTJ50 / Specialized brightening compound with corrosion inhibitors 30 to 45 minutes deep specular reflection, judged against a boundary sample
Automated rotary barrel tumbling machine model OBD-BJ160B with integrated control console and safety enclosure
Automated finishing machine with enclosed drum and programmatic touchscreen PLC console. For dedicated wheel finishing and multi-axis tumbling, facilities utilize enclosed rotary barrel tumbling machines featuring programmable forward/reverse rotation, variable speed drives, and rapid media drain ports.

The Stray Grit Contamination Hazard

The primary challenge in single-station wheel polishing is media cross-contamination:

  • A standard wheel polishing tub holds between 300 kg and 600 kg of media.
  • If a facility attempts to perform all three stages in a single bowl, every single pellet of coarse Stage 1 media must be evacuated before Stage 3 zirconia beads are charged.
  • The Catastrophic Failure Mode: If just one single 120# plastic cone remains trapped behind a drain baffle or bowl spring and enters the Stage 3 burnishing cycle, it will drag across the soft aluminum rim face under the high compressive pressure of the zirconia charge, carving deep spiral gouges across the mirror face. This scraps a $400 wheel in the final 5 minutes of processing.

Engineering Solutions for Media Evacuation:

  1. High-Capacity Pneumatic Discharge Ports: Production machines utilize bottom-tangential or side-wall pneumatic dump gates with aperture diameters > 150 mm, discharging 400 kg of media into receiving tote bins within 120 seconds.
  2. High-Pressure Flood Flushing: Automated internal spray rings blast high-volume water (80 L/min) through the empty bowl to flush all residual grit through the open dump valve before the next media grade is loaded via overhead hoist.
  3. Dedicated Cell Configurations (The OEM Standard): High-volume production plants avoid media changeover entirely by establishing a three-machine cell (Bowl 1: Coarse; Bowl 2: Fine; Bowl 3: Burnish). An overhead manipulator transfers the fixtured wheel between bowls in under 30 seconds.

For guidance on media selection and volumetric charging principles, review our vibratory tumbler media selection guide.

Takt-Time Optimization and Bottleneck Management

A conventional single-bowl vibratory cycle running from raw cast/machined state to mirror polish requires 4.5 to 6.0 hours per wheel. Under continuous 24-hour operation, a single machine yields only 4 finished wheels per day—barely enough for one passenger car.

To balance wheel finishing with upstream CNC machining lines and commercial delivery schedules, manufacturing engineers implement two cycle-compression techniques:

```

Cycle Compression Architecture:

Standard Vibratory Sequence (Total: 330 min): [Stage 1: Coarse 150 min] ──► [Stage 2: Fine 120 min] ──► [Stage 3: Burnish 45 min] ──► 6 Hours / Part

Optimized Hybrid Cell (Total: 75 min): [Upstream CNC Diamond-Cut Turn: 8 min] └──► [Stage 1 Pre-Blasted / Direct Fine Cut: 35 min] └──► [Stage 3 High-Energy Mirror Burnish: 30 min] ──► 1.25 Hours / Part

```

1. Upstream Pre-Machining and Surface Preparation

Allowing loose vibratory media to cut down heavy CNC turning ridges wastes hours.

  • Fine Diamond Facing: By optimizing the upstream lathe finishing pass (using polycrystalline diamond / PCD inserts at high feed rates to achieve an initial turned surface of finer than a roughing pass), Stage 1 plastic cutting time is cut from 150 minutes down to 30–45 minutes.
  • Localized Dry Pre-Blasting: For forged wheels with heavy forged parting lines or severe curb damage, spot pre-blasting with fine plastic media or agricultural grit strips heavy oxidized crusts in 2 minutes, bypassing the coarse vibratory grind.

Downstream Rinsing and Spin-Drying Integration

Once the mirror burnishing cycle concludes, aluminum wheels must be rapidly unmasked, rinsed with deionized water, and dried immediately. Allowing residual water drops to pool inside spoke pockets or valve bores causes permanent calcium drying stains and atmospheric oxidation spotting. High-volume wheel cells integrate heated centrifugal industrial dryers or automated clean-air blow-off tunnels, an operational requirement detailed in our analysis of why drying is a critical process step.

2. Multi-Spindle Planetary Rotation vs. Free Vibratory Drift

In basic vibratory bowls, the fixtured wheel is rotated slowly by an auxiliary overhead motor at 1 to 5 RPM while the bowl vibrates beneath it.

  • By increasing the spindle drive to a bi-directional servo motor that alternates rotation (clockwise for 60 seconds, counter-clockwise for 60 seconds) at 12 to 25 RPM, the relative shear velocity between the fluidized media and the wheel spokes increases dramatically.
  • This dynamic shear cuts Stage 1 and Stage 2 cycle times by 40% to 55%, achieving uniform spoke window coverage without shadowing.

For comprehensive strategies on line integration and production balancing, read mass finishing aluminum parts without smearing.

Environmental Health, Safety (EHS), and Aluminum Sludge Management

Finishing aluminum wheels generates thousands of grams of sub-micron aluminum swarf suspended in aqueous chemical compound. Unmanaged aluminum fines introduce severe chemical and explosion hazards to a factory floor.

1. Hydrogen Gas Generation Hazards

When finely divided aluminum particles react with water in an enclosed space, an exothermic reaction generates flammable hydrogen gas:

2Al + 6H_2O longrightarrow 2Al(OH)_3 + 3H_2uparrow

  • Risk: If wet aluminum swarf accumulates in an unventilated settling tank, closed sump, or pipe run, hydrogen gas pockets form rapidly. A maintenance grinding spark or electrical discharge can cause an explosive deflagration.
  • Engineering Control: All wastewater collection reservoirs must be open-topped, continuously ventilated with forced air, and classified with ATEX/NFPA-compliant non-sparking exhaust systems.

2. Sludge Separation Technology

Dumping raw vibratory wastewater into municipal drains is illegal and rapidly clogs industrial plumbing with hardened aluminum hydroxide cakes.

  • Automatic Paper-Band Filtration: Effluent from the wheel polishing tub drains continuously across an automated indexing paper-bed filter (filtering particles down to 25 – 50\ μm). The spent paper indexes forward automatically, discharging moist aluminum cake into sealed disposal drums.
  • High-Speed Centrifugal Decanters: For large facilities operating 4 or more wheel finishing machines, a two-phase centrifugal separator extracts solid aluminum particulate down to 5\ μm, clarifying the water and chemical compound for closed-loop recycling.

3. Chemical Compound pH Management

Aluminum is an amphoteric metal susceptible to rapid corrosion in both acidic and alkaline environments:

  • The Caustic Blackening Trap: If compound concentration drifts alkaline (pH > 8.5), the surface develops dark grey or black smut (insoluble aluminum hydroxide and intermetallic copper/silicon precipitates). Once caustic blackening occurs, it cannot be buffed off; the wheel must be chemically stripped in acid or re-machined.
  • The Acid Etching Trap: If pH drops below 5.5, aggressive intergranular etching attacks spoke fillets, creating micro-pores that ruin final mirror clarity.
  • Optimal Window: Automated dosing pumps must maintain compound concentration at 1.5% – 2.5%, buffering the recirculating solution strictly between pH 6.8 and 7.8 using formulations like compound-LC10.

For detailed chemical dosing principles across different alloys, consult metal compound: aluminium versus steel.

Heavy Commercial Truck Wheels (22.5" & 24.5"): Safety and Fatigue Standards

Finishing commercial forged truck wheels (such as standard 22.5 × 8.25 or 24.5 × 8.25 heavy-vehicle wheels) involves critical mechanical and regulatory constraints that do not exist in passenger car styling.

```

Critical Inspection Zones on Heavy Commercial Truck Wheels:

[Tire Bead Seat Radius: Wall thinning MUST NOT exceed 0.15 mm] ┌─────────────────────────┐ │ │ │ └──────────┐ │ │ [Outer Rim Flange] │ [Rim Well / Drop Center] │ │ │ └────────────────────────────────────┘ │ [Vent Hole / Hand Hole Fillets: Stress concentration zone — Micro-cracks must be detected before polishing]

```

1. High-Torque Heavy Fixturing

A forged commercial truck wheel weighs 23 kg to 26 kg bare. When loaded with centrifugal and hydrodynamic drag inside a high-speed fluidized media bed, the overturning moment exerted on the spindle drive exceeds 450 Ncdotm.

  • Standard passenger car chucks will fail catastrophically under this load.
  • Truck wheel polishing machines feature heavy-duty induction-hardened alloy spindles (minimum ⌀ 80 mm), supported by oversized dual taper roller bearings and powered by high-torque geared motors (minimum 7.5 kW to 11.0 kW drive power).

2. Tire Bead Seat Wall-Thinning Limits

Heavy commercial fleet wheels operate under high pneumatic tire pressures (100 – 120 PSI / 6.9 – 8.3 bar) supporting gross vehicle axle loads up to 10,000 kg.

  • Over years of highway service, road salt, moisture, and mounting friction cause severe pitting corrosion and bead-seat oxidation, leading to chronic tubeless tire air leaks.
  • The Regulatory Constraint: Commercial vehicle standards — including DOT (U.S. Department of Transportation), SAE J267, and ISO 7141 — mandate minimum rim section thicknesses.
  • The Processing Rule: Polishing must remove oxidation without degrading the critical bead seat profile. Total radial metal removal across all finishing stages must be controlled to ≤ 0.15 mm. If an operator aggressively grinds the bead seat to remove deep pitting, the rim wall thins past safe fatigue limits, creating an acute risk of explosive rim flange separation during highway transit.

3. Hand Hole (Ventilation Hole) Edge Conditioning

Commercial truck wheels feature 8 or 10 large ventilation openings in the wheel disc. These holes are prime stress-concentration zones where cyclical torsional fatigue cracks originate.

  • Abrasive media must achieve a continuous, smooth radial edge break (R0.5 – R1.0 mm) around every vent hole, eliminating micro-notches left by stamping or laser cutting.
  • Before any truck wheel is accepted for polishing, non-destructive testing (fluorescent dye penetrant inspection / PT or eddy current testing) must confirm that no fatigue micro-cracks exist in the vent hole fillets.

Shop-Floor Troubleshooting Matrix: Diagnosing Wheel Polishing Defects

Observed Defect Probable Root Cause Verification Method Corrective Engineering Action
Center Bore Out-of-Round / Enlarged (Wheel fails hub-centric mounting gauge) 1. Mandrel seal failure allowing abrasive slurry intrusion.<br>2. Radial mandrel expansion force excessive, plastically deforming bore. Measure bore diameter across 4 axes using internal three-point bore micrometers (+0.05 mm limit). Replace worn Shore 90A expanding polyurethane sleeve; verify mandrel pneumatic clamping pressure is within specified calibration (4.0 – 5.5 bar).
Orange Peel / Micro-Pitting on Outer Face (Surface shows wavy, dimpled texture rather than specular reflection) 1. Excessive vibratory amplitude or oversized zirconia media peening soft metal.<br>2. Acidic corrosion from stagnant wash solution. Inspect surface topography under 40× optical magnifier; check bath pH. Switch from large media to ⌀ 3 mm zirconia beads; reduce motor eccentric weight angle; verify compound delivery rate and maintain bath pH between 6.8 and 7.8.
Severe Spoke Shadowing (Face of wheel is polished bright, but vertical spoke sidewalls remain raw) 1. Media flow velocity insufficient to penetrate narrow spoke gaps.<br>2. Spindle rotation uni-directional, starving downstream pocket faces. Visual inspection under high-intensity inspection light; measure Ra on spoke interior sidewall. Implement programmed bi-directional spindle rotation (reversing direction every 60 s); substitute spherical media with angle-cut plastic triangles that wedge into tight spoke draft angles.
Dark Grey Discoloration / Black Ash (Aluminum develops unremovable dark film post-cycle) 1. Chemical compound pH > 8.5 causing caustic dissolution.<br>2. Fine aluminum swarf packing into ceramic media micro-pores. Test drain water pH with calibrated digital meter; inspect media surface texture. Immediately dump bath; flush system with clean water; recharge with neutral compound-LC10; run a 20-minute media self-cleaning cycle without parts.
Lodged Media in Valve Hole or Rim Recesses (Pellets wedged tightly, requiring manual chisel removal) 1. Media diameter matches valve stem hole (⌀ 11.5 mm) or spoke drainage slots (± 10%).<br>2. Media worn down to critical wedging size. Check wedged stone dimensions against part drawing. Install dedicated elastomeric masking plugs in valve holes before loading; periodically screen media charge to discard fractured or worn pellets.

For volumetric loading practices and fluid dynamics, review loading ratio: the variable that decides yield.

Boundary Limitations: When Mass Finishing Does Not Apply to Wheels

Mass finishing vibratory bowls and barrel equipment are highly effective for surface conditioning, but they are not universal repair tools. Certain structural and metallurgical wheel conditions cannot be resolved in mass finishing equipment:

  1. Severe Curb Rash and Deep Gouging (> 1.5 mm depth):

Vibratory finishing removes micro-burrs and levels minor machining textures (0.05 – 0.15 mm depth). Attempting to polish out deep curb gouges via mass finishing will wash away surrounding spoke geometry and ruin structural wheel balance. Deep gouges require mechanical TIG weld buildup followed by precision CNC lathe profiling prior to decorative polishing.

  1. Structural Radial Runout or Lateral Bent Rims:

An out-of-round or bent wheel cannot be corrected by polishing. Rims with structural bend > 0.5 mm must be mechanically straightened on a hydraulic wheel repair machine with localized induction heating before surface treatment.

  1. Ultra-Lightweight Forged Magnesium Racing Wheels:

Magnesium alloys are violently reactive with aqueous solutions. Processing magnesium in standard water-based vibratory equipment risks severe galvanic oxidation, pitting, and dangerous hydrogen gas evolution. Magnesium wheels require specialized non-aqueous hydrocarbon or dry organic polishing mediums (such as treated walnut shell granules) running in sealed inert atmospheres.

  1. Clear-Coat Stripping of Powder Coated Wheels:

Vibratory tumbling media cannot efficiently strip thick OEM automotive clear powder coat (80 – 150\ μm thick). The tough polyurethane or polyester film cushions abrasive impact, resulting in hours of wasted cycle time. Wheels must be chemically stripped in heated benzyl alcohol or immersion stripping baths before entering mass finishing equipment.

Verified Machine Specifications and Custom Manufacturing Capabilities

All industrial mass finishing machinery and automated polishing stations manufactured by our facility in Xiamen, China (established in 1992) are produced under certified industrial standards:

  • European CE Machinery Compliance: Fully certified under CE Machinery Directive across all equipment lines:
  • Certificate M.2023.206.C88120 (Horizontal, Vibratory, and Barrel platforms; valid through 2028-07-24; reports DTT230706S003 / S004) covering models including ZL150, ZL300, ZL450, HG70A, WFX50B, LLG40, LLQ120, YH-680D, ZL150, YG350, YG450, HBPG-01, HBPG-02, and GSLX-120.
  • Certificate M.2023.206.C88121 (Vertical and Rotary platforms; valid through 2028-07-24; reports DTT230706S005 / S006) covering models including LX80B, CJS480A, CJS320, CJG480A, CJG320, BJ160B, BLG400, and BLG200 (21 verified machine models total).
  • ISO 9001 Quality Management Certification: Current valid Certificate 00726Q01571R001 issued by Zhongjian Certification Co., Ltd. (valid through 2029-06-02) covering the production and sales of surface finishing and polishing machinery.
  • Intellectual Property: Supported by 24 granted Chinese intellectual property rights, including 1 invention patent, 17 utility model patents, and 6 design patents. For criteria on validating factory credentials, see how to vet deburring and finishing machine manufacturers.

OEM Custom Fixture and Line Integration Services

Because wheel geometries, offset depths (ET), pitch circle diameters (PCD), and hub bore configurations differ across passenger car, motorsport, and commercial truck applications, we design and build customized fixturing solutions and automated finishing cells tailored to customer engineering drawings.

We do not supply off-the-shelf catalog wheel machines with unverified universal chucks. What that takes is a decision for the part rather than for the catalogue; the fixture question is settled against the part, target cycle times, and alloy specifications to configure dedicated pneumatic expansion mandrels, automated media changeover dump chutes, and matching chemical dosing systems.

To submit wheel drawings for trial verification or discuss customized finishing cell engineering, connect directly with our application specialists through our technical contact portal.

#+86-592-2381506

Email : info@surface-polish.com

Headquarters address : No. 31, Xinchang Road, Xinyang Industrial Zone, Haicang District, Xiamen

click here to leave a message

Leave A Message
If you are interested in our products and want to know more details,please leave a message here,we will reply you as soon as we can.

Preparing secure enquiry form…

Home

Products

whatsapp

contact